Sprache
:
Trifunctional alicyclic epoxy resin YLCE-186 is a mixed epoxy resin with one alicyclic epoxy group and two glycidyl esters, CAS 25293-64-5. The product page lists EEW 100–115 g/eq, viscosity 2000–4000 cps at 25 °C, APHA max. 50 and volatiles max. 1 % for grade YLCE-186, the purer of the two grades.
The product page describes the molecule as one cycloaliphatic epoxide plus two glycidyl esters. Of the two reactive sites, the glycidyl ester is the faster, so reactivity exceeds that of a plain cycloaliphatic grade at similar viscosity.
The same page states cure with anhydrides, amines and cationic initiators. Three reactive sites per molecule raise crosslink density relative to the 125–135 g/eq YLCE-2021 diepoxide.
Table 1. Values as published on the YLCE-186 product page; the last row gives the difference the page itself states.
| Item | YLCE-186C | YLCE-186 |
| Appearance | Light yellow liquid | Colorless to light yellow liquid |
| Color, APHA | max. 50 | max. 50 |
| Viscosity, cps at 25 °C | 2000–5000 | 2000–4000 |
| Epoxy equivalent weight, g/eq | 110–125 | 100–115 |
| Volatiles, % | max. 1 | max. 1 |
| Difference stated by the page | Lower price | High purity |
The diglycidyl ester of 4,5-epoxytetrahydrophthalic acid is C14H18O7 at 298.29 g/mol, so three epoxy groups correspond to 99.4 g/eq. The published 100–115 g/eq for this trifunctional alicyclic epoxy resin implies 2.6–3.0 groups per molecule, and the label holds. Where a measured EEW implies fewer groups, dose from EEW.
Amine dosage follows 100 × AHEW ÷ EEW, with AHEW from the hardener page. YLH-9101 records AHEW 92 g/eq and 48 phr against a liquid bisphenol A resin at EEW 190. The lower EEW of these grades pushes the same hardener to 80–92 phr.
Table 2. phr calculated from the published EEW and the published AHEW of YLH-9101; the anhydride columns use an AEW of 168 g/eq derived from the molecular weight of MHHPA, CAS 25550-51-0. All values are theoretical.
| EEW, g/eq | YLH-9101, phr | MHHPA at 1.00, phr | MHHPA at 0.85, phr |
| 100 | 92 | 168 | 143 |
| 107.5 | 86 | 156 | 133 |
| 115 | 80 | 146 | 124 |
The 0.85 anhydride column is a common starting ratio for castings, since full stoichiometry can leave unreacted anhydride in a rigid matrix. Near 90 phr of amine on a 100 g mix is a substantial exotherm. The page publishes no gel time for either grade, so confirm against the TDS before scaling a batch.
YLCE-186C is the lower-cost grade at higher EEW and a wider viscosity band; YLCE-186 is the high-purity grade at 100–115 g/eq. Both are held at APHA max. 50, so the difference shows in appearance and price, not in the color number.
For insulating parts the electrical and electronic application note sets out the requirements. A 500 g sample of YLCE-186, the current TDS, and one casting at 0.90 of stoichiometry are the next step.