Heim Blog

Non-Crystalline Epoxy Resin: Why YLE-128R Survives Winter Freight

Non-Crystalline Epoxy Resin: Why YLE-128R Survives Winter Freight
November 30, 2026

Non-crystalline epoxy resin is a liquid bisphenol A grade whose EEW band is widened to 185-220 g/eq in YLE-128R and 205-240 g/eq in YLE-128S. A wider band slows the lattice that clouds standard resin near 5 °C, and viscosity reaches 25,000 mPa·s. Phr moves 16% across the band, so dosing is per drum.

Glass jar of clear pale amber liquid epoxy resin beside a condensate-covered steel drum lid on a cold warehouse shelf

Figure 1. Clear liquid bisphenol A epoxy resin beside a condensate-covered drum lid: clarity at low temperature is the property under test.

1. Introduction

The complaint rarely starts in a laboratory. It starts in a shed that fell to 2 °C overnight, or in a container that crossed a mountain pass in January.

A standard liquid bisphenol A resin leaves the plant water-clear at 25 °C and arrives hazy, with grit in the drum head.

Standard liquid bisphenol A epoxy resin such as YLE-128 sits at 184-190 g/eq on the same product page, about 0.10 to 0.14 repeat units per molecule. That band is narrow enough to pack, and one nucleus seeds the rest.

YLE-128R and YLE-128S widen the band to 185-220 and 205-240 g/eq. This report separates symptom from cause, then prices the trade-off in phr.

2. Materials and Methods: What a Non-Crystalline Epoxy Resin Specification Contains

Both grades are bisphenol A diglycidyl ether. The backbone does not change; only the EEW distribution and the viscosity band move.

2.1 Product identification and specification

Table 1 collects what Yolatech publishes. YLE-128R and YLE-128S share the bisphenol A epoxy resin product page with YLE-127, YLE-128 and YLE-130.

Table 1. Product identification for YLE-128R and YLE-128S, from the bisphenol A epoxy resin product page and the 2026 catalog, page 3.

Item

Information

Chemical name

Bisphenol A diglycidyl ether

Appearance

Clear pale liquid, color max. 1 Gardner

EEW

185-220 g/eq / 205-240 g/eq

Viscosity at 25 °C

11,000-25,000 mPa·s / 12,000-25,000 mPa·s

Hydrolyzable chlorine

printed as 2% for YLE-128R / 5,000 ppm for YLE-128S

Catalog application

Composite, adhesives, coating, flooring

CAS number

not printed on the page, confirm on the COA

Table 2 places both grades beside YLE-128, the grade they replace. The EEW span row carries the argument.

Table 2. Property comparison of YLE-128R, standard YLE-128 and YLE-128S.

Property

YLE-128R

YLE-128

YLE-128S

EEW, g/eq

185-220

184-190

205-240

EEW span, g/eq

35

6

35

Viscosity at 25 °C, mPa·s

11,000-25,000

11,000-15,000

12,000-25,000

Color as printed

1 Gardner

50 APHA

1 Gardner

Hydrolyzable chlorine

2% as printed

500 ppm

5,000 ppm

2.2 Test methods and data sources

EEW is determined by titration according to ASTM D1652, with ISO 3001 as an equivalent route. Viscosity is quoted at 25 °C, and color follows ASTM D1544.

No wet-lab work was performed. Each physical value is a page or catalog figure, and each phr value is calculated. Water content, if it matters, follows ASTM E203.

3. Results and Discussion: Why a Non-Crystalline Epoxy Resin Resists Seeding

Crystallization needs order, and order needs a narrow distribution. Widen the distribution and the melting range drops.

3.1 Structure and reactivity

For a bisphenol A diglycidyl ether oligomer, EEW follows 170 + 142n, where n is the average repeat count. EEW 185 gives n = 0.11 and EEW 220 gives n = 0.35.

That spread is the mechanism. Mixed homologues cannot stack on one lattice, the melting range broadens downward, and the driving force for nucleation shrinks.

Nucleation is slowed, not removed. A seeded drum held at 0 °C still clouds.

Viscosity is the price. YLE-128R reaches 25,000 mPa·s against 15,000 mPa·s, a 67% higher ceiling, because higher oligomers carry more mass.

Reactivity moves the other way. EEW 220 needs 82.7 phr of YLH-3002 where EEW 185 needs 98.4 phr, so one drum can shift the mix ratio by 16%.

3.2 Comparison with alternative systems

Table 3 sets YLE-128R against the standard grade and liquid bisphenol F, the usual low-viscosity answer.

Table 3. YLE-128R against two alternatives on the properties that decide cold-storage behaviour.

Property

YLE-128R

YLE-128

YLE-170 (liquid BPF)

EEW, g/eq

185-220

184-190

160-180

Viscosity at 25 °C, mPa·s

11,000-25,000

11,000-15,000

2,000-5,000

Color as printed

1 Gardner

50 APHA

max. 1 Gardner

Hydrolyzable chlorine

2% as printed

500 ppm

500 ppm

Crystallization risk in cold storage

reduced by band width

high

high on low-chloride grades

Effect on mixed viscosity

higher than standard

baseline

much lower

Bisphenol F buys flow, 2,000-5,000 mPa·s against 11,000-25,000 mPa·s, but the catalog labels its low-chloride grades crystalline epoxy resin, so cold storage still bites. If flow outranks clarity, liquid bisphenol F resin wins; if clarity outranks flow, it does not.

4. Formulation and Dosage Calculation

Hardener mass follows phr = 100 × AHEW ÷ EEW, with AHEW from the hardener data sheet and EEW from the resin lot.

Table 4 runs the formula at the mid-point of each band for three hardeners.

Table 4. Hardener demand in phr, calculated from AHEW and the mid-point EEW of each band.

Hardener (AHEW, g/eq)

YLE-128 at EEW 187

YLE-128R at EEW 202.5

YLE-128S at EEW 222.5

YLH-3002 (182)

97.3 phr

89.9 phr

81.8 phr

YLH-5022 (175)

93.6 phr

86.4 phr

78.7 phr

YLH-6005 (95)

50.8 phr

46.9 phr

42.7 phr

YLH-3002, whole band

95.8-98.9 phr

82.7-98.4 phr

75.8-88.8 phr

Read the bottom row before ordering. YLE-128R carries 15.7 phr of movement inside one band.

Dose at 89.9 phr and a 220 g/eq lot arrives with 8.7% excess amine; the network plasticizes and a damp wall blushes. A 185 g/eq lot leaves the same mix 8.6% short.

Titrate each lot. A phr copied from the last drum is an assumption, not a specification.

5. Processing Notes and Operating Window

Heat fixes the symptom if the drum is warmed evenly and stirred before sampling.

• Warm to 45-50 °C, not 70 °C. Above 60 °C the color drifts and the drum skin scorches.

• Roll or stir the whole drum. Clear liquid decanted off a crystalline heel carries seeds forward.

• Hold the mixed system above 15 °C. Below that, YLE-128S tops out near 25,000 mPa·s and air stops rising.

• Filter if grit shows. A 200 µm screen catches the crust without stripping resin.

Table 5. Field symptoms, their causes, and the action that clears them.

Symptom

Likely cause

Action

haze at 5 °C, clear at 25 °C

incipient crystallization

warm to 50 °C, stir, retest

grit in the drum head

settled crystals

roll the drum, do not decant

solid ring on the wall

nucleation at a cold wall

melt the ring, homogenise

viscosity above 25,000 mPa·s

cold resin, not a spec shift

recheck at 25 °C first

blush on a damp wall

amine excess from a low-EEW lot

retitrate EEW, recalculate phr

Steel drum of amber epoxy resin opened in a cold plant with crystalline skin on the surface and a band heater clamped around it

Figure 2. A drum opened after cold storage: the surface skin is melted and homogenised before any sample is taken.

6. Applications: Where the Non-Crystalline Grades Pay Off

Four application areas take most of the volume, each failing differently.

6.1 Cold-climate flooring and self-levelling

Flooring sets the hardest viscosity demand: self-levelling needs flow at 15 °C, and the 25,000 mPa·s ceiling leaves little room.

Dose 89.9 phr of YLH-3002 at EEW 202.5. The failure mode is a cold pour that will not close a trowel mark.

6.2 Composite wet lay-up and filament winding

Wet lay-up runs YLE-128R at 89.9 phr with YLH-3002 or 86.4 phr with YLH-5022 polyamide hardener, depending on pot life.

Risk sits in a batch warmed only at the wall: the lay-up cures unevenly and shows white streaks.

6.3 Structural adhesives

Adhesives want the higher-EEW end, where YLE-128S at 222.5 g/eq gives 81.8 phr with YLH-3002 modified cycloaliphatic amine and a longer open time.

The 5,000 ppm chlorine level rules YLE-128S out of electronic bonds; construction adhesives do not care.

6.4 Protective coatings and winter primers

Coatings accept the viscosity and gain cold-weather clarity; haze shows in a gloss finish.

Pair with YLH-5022 at 86.4 phr for flexibility, or YLH-6005 at 46.9 phr where a 5 °C cure matters more than pot life.

Table 6. Application, dose and failure point for the two grades.

Application

Dose

Function

Failure point

cold-climate flooring

89.9 phr YLH-3002

flow at 15 °C

cold pour that will not level

wet lay-up composite

86.4 phr YLH-5022

wet-out at workable viscosity

uneven cure after partial remelt

structural adhesive

81.8 phr YLH-3002 on YLE-128S

longer open time

amine excess on a low-EEW lot

protective coating

86.4 phr YLH-5022

gloss and clarity

haze from a crystalline heel

winter primer

46.9 phr YLH-6005

fast set at 5 °C

short pot life in a warm shop

Clear amber epoxy resin drawn across a woven glass fibre laminate with a metal squeegee on a workshop bench

Figure 3. Clear resin drawn across a glass laminate: haze from a crystalline heel shows as white streaks under the surface.

7. Limitations and Material Verification

7.1 Known limits and unsuitable uses

Two limits are hard. YLE-128S carries 5,000 ppm hydrolyzable chlorine, which puts it outside electronic potting; the low-chloride 128K, 128L and 128P grades cover that work.

A widened band suppresses crystallization, it does not abolish it. Weeks below 0 °C still produce nuclei.

Stoichiometry is the quieter limit. EEW 185-220 spans 19%, so one phr fits one lot and misses the next.

One chlorine figure needs care. The product page and the catalog both print 2% for YLE-128R, which does not match the ppm scale used on the same row, so treat it as unverified until a COA confirms it.

A second discrepancy concerns YLE-128. The catalog prints 184-194 g/eq against 184-190 on the page, so this report uses the page value; a COA settles it.

7.2 Incoming verification, packaging, storage and safety

Verify EEW on every lot according to ASTM D1652, and hold a retained sample at 5 °C for seven days to watch for haze.

Storage above 15 °C avoids most incidents; a heated room costs less than a returned drum. Read the current TDS, MSDS and COA before reformulating.

• Check the drum head on receipt. A crust means the drum crossed a cold leg.

• Do not stand IBCs on a concrete floor in an unheated shed; the base is the coldest point.

• Keep uncured resin off skin. Bisphenol A epoxy is a sensitiser; gloves are the control.

8. Frequently Asked Questions

At what temperature does liquid epoxy resin crystallize?

Standard liquid bisphenol A resin starts to crystallize near 0-10 °C, fastest a few degrees below its melting range. YLE-128R widens that window, and does not close it.

Is YLE-128R a different molecule from YLE-128?

No. Both are bisphenol A diglycidyl ether. YLE-128R carries a wider oligomer distribution, EEW 185-220 g/eq against 184-190 g/eq, and that distribution is the product.

Can a crystallized drum be recovered?

Yes, by warming to 45-50 °C and rolling until the ring and the heel are gone. Decanting the clear top layer leaves the seeds behind and the batch clouds again within days.

Which grade needs more hardener, YLE-128R or YLE-128S?

YLE-128R. At EEW 202.5 g/eq it takes 89.9 phr of YLH-3002, while YLE-128S at 222.5 g/eq takes 81.8 phr, a 10% difference in hardener mass.

Does the wider EEW band change cured properties?

Slightly. Higher oligomer content lowers epoxy content per kilogram, so a 185 g/eq lot cures harder than a 220 g/eq lot of the same grade.

Is YLE-128S suitable for electronic potting?

No. At 5,000 ppm hydrolyzable chlorine it is a general-purpose grade. The 128K, 128L and 128P grades are the low-chloride options for potting.

9. Conclusions

YLE-128R and YLE-128S hold clarity through cold freight by widening the EEW band to 185-220 and 205-240 g/eq. The cost is a 25,000 mPa·s ceiling and a phr that moves 16% across the band.

Dosing from one fixed phr is the failure that follows. Titrate each lot, warm the drum evenly, and stir before sampling.

Where flow outranks clarity, liquid bisphenol F remains the better trade.

10. References

Yolatech product page, bisphenol A epoxy resin: https://www.yolatech.com/bisphenol-a-epoxy-resin (accessed 2026-11-30).

Yolatech Technical Data Sheet for YLE-128R and YLE-128S, bisphenol A diglycidyl ether (available on request).

Yolatech Certificate of Analysis (COA) for YLE-128R, bisphenol A diglycidyl ether (available on request).

ASTM D1652, epoxy content of epoxy resins (EEW).

ISO 3001, determination of epoxy equivalent.

ASTM D1544, Gardner color of transparent liquids.

ASTM E203, water content by Karl Fischer titration.

eine Nachricht hinterlassen

eine Nachricht hinterlassen
Wenn Sie an unseren Produkten interessiert sind und weitere Einzelheiten erfahren möchten, hinterlassen Sie bitte hier eine Nachricht. Wir werden Ihnen so schnell wie möglich antworten.
Einreichen

Heim

Produkte

WhatsApp

Kontaktiere uns