  YLH-3054 is a chemical-resistant epoxy hardener developed for heavy-duty epoxy corrosion protection. This modified polyamine epoxy hardener offers outstanding chemical resistance against most organic acids, alcohols, edible oils, fats, and solvents. Its chemical resistance is further improved when combined with phenolic novolac epoxy resin, supporting epoxy novolac pipeline coating formulations where greater chemical resistance is required.

  As a high-temperature epoxy hardener for pipeline coatings and internal linings, YLH-3054 combines chemical resistance, early water resistance, thick-film crack resistance, and high-temperature performance in one epoxy curing system. The evaluation below covers thermal aging at 200°C for 168 h and thermal cycling from 230°C to -60°C. The data are relevant to petroleum pipeline coating development and to the use of this epoxy hardener for steel pipe coating and other high-temperature anticorrosive coating systems.

 

Advantages for Pipeline Corrosion Protection

Chemical-Resistant Epoxy Hardener for Pipeline Corrosion Protection

Chemical tank lining; Pipeline internal lining; Heavy-duty steel anti-corrosion primers.

 

Early Water Resistance and Thick-Film Performance

Excellent early water resistance, good flexibility, providing good crack resistance in thick film applications.

Cathodic Protection Compatible Coating Systems

Excellent compatibility with cathodic protection systems. Suitable for the design of related pipeline corrosion-protection systems.

High-Temperature Pipeline Coating Performance

After 200°C/168 h exposure and thermal cycling from 230°C to -60°C, the tested system showed no chalking, cracking, or peeling.

 

Typical Properties

Appearance

Light yellow liquid

Viscosity, mPa.s@25°C

0-100

Amine value, mg KOH/g

280-320

AHEW, g/eq

160

Added Weight, PHR

75-85

 

To evaluate YLH-3054 as an epoxy curing agent for pipeline coating applications, Formulation A was compared with the control formulation for curing, adhesion, and high-temperature performance. YLH-3054 was added separately as the curing component (Part B) at 20.8 g. The formulation and test results are shown below.

 

 

Formulation A (YLH-3054 Curing System)

No.

Raw Material

Amount

1

Xylene

13.5

2

n-Butanol

3.4

3

YLEP-638

23.5

4

Talc

19.8

5

Yellow Iron Oxide

1

6

Barium Sulfate

31.9

7

Titanium Dioxide

6

8

Carbon Black

0.1

9

Ultra

0.8

Hardener

YLH-3054 (Part B)

20.8 g

 

1. BK Drying

Item

Surface Dry (25°C)

Hard Dry (25°C)

Formulation A

2h

3h

Control Formulation B

1.5

≥6h

At 25°C, Formulation A reached surface dry in 2 h and hard dry in 3 h. The control reached surface dry in 1.5 h but required ≥6 h for hard dry. Although Formulation A was slightly slower to reach surface dry, it completed effective crosslinking much faster.

Figure 1  BK Drying Test

 

 

2. Pull-off Adhesion for Pipeline Coatings

Item

Pull-off Adhesion (Before) / MPa

Pull-off Adhesion (After) / MPa

Formulation A

23.32  23.03

21.63    18.36

Control Formulation B

7.62   8.22

21.14    21.08

Before heat exposure, pull-off adhesion of Formulation A was 23.32/23.03 MPa, compared with 7.62/8.22 MPa for the control. This shows that Formulation A developed higher initial adhesion under ambient curing conditions.

Note: "Before" and "After" refer to before and after baking at 200°C for 168 h.

Figure 2  Adhesion Test

 

3. Thermal Aging Performance at 200°C

Item

Film Surface Condition After Baking at 200°C for 168 h

Formulation A

Discoloration observed; no chalking, cracking, or peeling.

Control Formulation B

Discoloration observed; no chalking, cracking, or peeling.

After baking at 200°C for 168 h, both coatings showed discoloration but no chalking, cracking, or peeling, and the coating films remained intact.

Figure 3  Thermal Aging Test

 

 

4. Thermal Cycling Performance

Item

Film Surface Condition After 3 Thermal Cycles of 230°C (16 h) and -60°C (8 h)

Formulation A

Discoloration observed; no chalking, cracking, or peeling.

Control Formulation B

Discoloration observed; no chalking, cracking, or peeling.

After 3 thermal cycles between 230°C (16 h) and -60°C (8 h), both coatings showed discoloration but no chalking, cracking, or peeling, demonstrating stable resistance to thermal cycling.

Figure 4  Thermal Cycling Test

 

5. Conclusion

  Comparative results show that the main strengths of Formulation A are faster hard-dry development and earlier adhesion build. Its surface-dry time was 2 h, slightly longer than the control at 1.5 h, but Formulation A reached hard dry in 3 h while the control required ≥6 h. In addition, pull-off adhesion after ambient cure reached 23.32/23.03 MPa for Formulation A, compared with 7.62/8.22 MPa for the control.

  After baking at 200°C for 168 h and thermal cycling between 230°C and -60°C, neither coating showed chalking, cracking, or peeling. These results indicate that Formulation A achieved a good balance among curing efficiency, initial adhesion, and coating film integrity under high-temperature conditions.

 

eine Nachricht hinterlassen

eine Nachricht hinterlassen
Wenn Sie an unseren Produkten interessiert sind und weitere Einzelheiten erfahren möchten, hinterlassen Sie bitte hier eine Nachricht. Wir werden Ihnen so schnell wie möglich antworten.
Einreichen

Heim

Produkte

WhatsApp

Kontaktiere uns